Induction Hardening Surgical Knife Blades
Views Send Enquiry
   Objective Harden a 4″(101.6mm) section of a Stainless Steel surgical blade measuring 7″ (177.8mm) long. Hardness should be 48 to 53 Rockwell C on the blade after processing.
  Material 420 Stainless Steel Surgical Blades measuring 7″(177.8mm)
  long, 1/4″(6.35mm) wide at the shank, and 0.085″ (2.2mm)
  thick at the blade.
  Temperature 1850ºF(1010ºC)
  Frequency 365 kHz
  Equipment •Power of 4.5 kW induction heating system equipped with a remote workhead including one (1) capacitor equaling 1.2 μF
  • An induction heating coil designed and developed specifically for this application.
  Process A two turn helical coil with an internal quartz tube designed to scan the length of the blade is used to heat the blade to 1850ºF (1010ºC) to achieve the desired hardness.
  Results/Benefits Induction heating provides:
  • Flameless process
  • Improved production rate
  • Consistent & repeatable results
   
  
Related Content
 - Air Cooled clamp coil (half-open coil) for preheating gas pipeline
 - induction coating by air cooled clamp induction coil
 - Remove plastic coating from steel tubes by Induction Heating
 - Releasing Fixture by Induction Heating
 - U shape air cooled induction coil by UM-100C-HF for pipeline preheating
 - induction quenching with custom-design inductor
 - induction brazing diamond segment
 - induction brass soldering copper plate_2
Hot
 
 induction hardening axle (shaft) by 100KW induction heater
 
 induction quenching axle (shaft) by 160KW induction heater
 
 induction hardening inner surface (inwall)
 
 Induction Hardening Harvestor Combined Finger
 
 Induction Hardening Harvestor Combined Blade
 
 workpiece for induction hardening
 
 induction hardening veterinary instrument
 
 induction hardening surgical device

Newest Comment
No Comment
Post Comment