Induction Soldering Fiber Optic
Views Send Enquiry
Objective To heat a fiber optic housing to 400°F within 10 seconds for avsoldering application, to form a hermetic seal
Material Gold-plated aluminum housing, solder preform ring and flux
Temperature 400 ºF
Frequency 267 kHz
Equipment Power of 10kW power supply, remote heat station with a specially designed induction coil.
Process A specially designed, two-turn plate concentrator coil was used to provide uniform heat to the joint area. Initial tests were conducted to establish a heating pattern and time-totemperature.
The goal was to deliver uniform heat to the lid as well as to the housing. One solder preform was applied at the
joint and flux was applied to the joint surface. A ceramic fixture was used to maintain uniform pressure on the lid and keep it from buckling during the heat cycle. RF power was applied for 10 seconds, causing the solder to melt and flow.
Results Consistent and repeatable results were achieved with the Power of 10kW power supply and an 10-second heat cycle.
The solder flowed evenly and bonded the lid to the housing without any visible voids.

Soldering Fiber Optic
Related Content

Air Cooled clamp coil (half-open coil) for preheating gas pipeline

induction coating by air cooled clamp induction coil

Remove plastic coating from steel tubes by Induction Heating

Releasing Fixture by Induction Heating

U shape air cooled induction coil by UM-100C-HF for pipeline preheating

induction quenching with custom-design inductor

induction brazing diamond segment

induction brass soldering copper plate_2









Newest Comment
No Comment
Post Comment